Elastomer Systems>>Effects of Curative

All physical properties of Vastsky elastomers are sensitive to curative level.

The curative level is often expressed as % Theory.

100% theory for example means the curative level used is the exact amount required to react with the prepolymer.

The table shows how Physical Properties vary with % Theory.

Physical PropertyChange
HardnessRemains unchanged between 85-100% theory .
Tensile StrengthMaximum physical properties achieved between 90-95% theory.
Tear StrengthMaximum properties at 100-105% theory. Significantly lower outside the range.
Abrasion ResistanceRemains relatively unchanged between 85-105% theory. Slightly better at 100-105% theory.
Flex LifeMaximum property at 100-105% theory.
ElongationMaximum at 100-105% theory.
Compression set & heat resistanceBest at 85-95% theory.